Nd:YAP

CRYTUR grows neodymium doped yttrium aluminium perovskite (Nd:YAP) crystals using the Czochralski growth method. A special protective atmosphere applied during crystal growth and post growth annealing result in a very good lasing efficiency of our crystals. Our production line covers crystal growth, machining and coating technologies.

Technical parameters

Technical parameters

Our standard production of Nd:YAP laser rods includes Nd dopant concentrations from 0.25 % up to 1.1 at. % of Nd/Y.

Nd:YAP laser rods with 0.7 at. % Nd/Y are typically used for CW and 0.9 at. % Nd/Y for pulsed lasers, both with the “b” orientation.

The threshold and slope efficiency of Nd:YAP at 1079 nm are comparable to those of Nd:YAG at 1064 nm. Rods cut along the “b” axis are suited for most of applications. 

Linear polarization, no thermal birefringence and easy generation of 1.3 µm wavelength are the main advantages of this material.

The 1340 nm emission wavelength of Nd:YAP has higher absorption in water and bodily fluids in comparison with the 1319 nm emission wavelength of Nd:YAG. 

effect of beam walk-off is eliminated and the conversion efficiency is increased compared to angular phase-matching.

Non critical phase matching in α-cut KTP

Taking into account the polarized output beam, Nd:YAP can be advantageously utilized in lasers with electro optic cells or harmonic generators. The wavelength of 1079 nm emitted by Nd:YAP can realize type II non-critical phase matching in an α-cut KTP crystal, where the effect of beam walk-off is eliminated and the conversion efficiency is increased compared to angular phase-matching.

Nd-YAP-PM-angle.jpeg

Material properties

Host Yttrium aluminium perovskite (YAlO3)
Dopant Nd3+
Crystal structure orthorhombic - Pbnm
Unit cell dimensions (Pbnm notation) a0= 0.518 nm
b0= 0.531 nm
c0= 0.736 nm
Refractive index at 1064 nm 1.914 (na)
1.925 (nb)
1.940 (nc)
Thermal expansion coefficient ||a: 9.5 x 10-6 / K
||b: 4.3 x 10-6 / K
||c: 10.8 x 10-6/ K
Thermal Conductivity 11 W/m K
Density 5.35 g/cm3
Hardness by Mohs 8.5
Fluorescent lifetime (1% Nd) 170 µs
Linear dispersion δn/δT [10-6K-1] 9.7 (na)
Laser wavelengths 4F3/2→4I9/2 930 nm
4F3/2→4I11/2 1079 nm
4F3/2→4I13/2 1340 nm
4F3/2→4I13/2 1432 nm

 

Emission cross sections of Nd:YAP in dependence on its crystallographic orientation.

(Ref. A. A. Kaminskii, Laser Crystals, New York: Springer Verlag 1981).

Wavelength [nm] Emission cross section [10-19 cm2]
a-cut b-cut c-cut
1079 2.05 1.76 1.38
1340 1.13 0.97 0.78
1432   0.34  

The main absorption line of the Nd:YAG crystal occurs at 808 nm. In case of Nd:YAP the peak of the absorption depends on crystallographic direction on Nd:YAP and polarization.

Absorbtion spectrum of Nd:YAP

Nd-YAP-absorbtion-spectrum-c-cut-polarized.jpeg Nd-YAP-absorbtion-spectrum-b-cut-polarized.jpeg
Nd-YAP-absorbtion-spectrum-unpolarized.jpeg  

Contact us